Casi el 90 % del betún asfáltico se utiliza en la construcción de carreteras, mientras que el porcentaje restante se emplea principalmente en techados.

Betún asfáltico Especificación

PARAMETERUNITTEST METHOD20/3030/4550/7070/100160/220
Penetration at 25°C0.1 mmDIN EN 142620 to 3030 to 4550 to 7070 to 100160 to 220
Ring and ball softening point°CDIN EN 142755.0 to 63.052.0 to 60.046.0 to 54.043.0 to 51.035.0 to 43.B0
Flash point°CEN ISO 2592≥ 240≥ 240≥ 230≥ 230≥ 220
Solubility%DIN EN 12592≥ 99.0≥ 99.099.0≥ 99.0≥ 99.0
Penetration indexDIN EN 12591,NRNRNRNRNR
Annex A
Kinematic viscosity at 135°Cmm²/sDIN EN 12595NRNRNRNRNR
Dynamic viscosity at 60°CPa × sDIN EN 12596NRNRNRNRNR
Fraass breaking point°CDIN EN 12593≤ -5≤ -8≤ -10≤ -15
Resistance to hardening at 163°C:DIN EN 12607-1
Residual penetration%DIN EN 1426≥ 55≥ 53≥ 50≥ 46≥ 37
Increase in ring and ball softening point°CDIN EN 1427≤ 8≤ 8≤ 9≤ 9≤ 11
Mass change%DIN EN 12607-1≤ 0.5≤ 0.5≤ 0.5≤ 0.8≤ 1.0

    Rellene el formulario para realizar una solicitud

    Datos de contacto:

    — campos obligatorios